MMM-A-1617B
4.6.3 Dead load (Type II). Three specimens shall be prepared in
accordance with 4.6.2.1.2, and conditioned as specified in 4.5.1. Within 24
hours after completion of conditioning, the samples shall be placed in a
circulating air oven at a temperature of 70°± 1°C (158°± 2°F). A 0.9 kg (2
lbs.) weight shall be suspended from the loose end of the duck, in a manner
which will apply the load at an angle of 90° to the aluminum strip. The
specimens shall be maintained at the above temperature for 24 hours, after
which they shall be removed from the oven and examined for compliance with
3.3.2.
4.6.4 Brushability. Brushability shall be evaluated during the
preparation of the strip adhesion specimens (see 4.6.2) and shall comply with
the requirements of 3.3.3.